JPEN

SPEC OF CEMENT
セメントのスペック

Report of tests on Ordinary Portland Cement

Physical Tests

Density   g/cm2 3.15  
Fineness: Air permeability test   cm2/g 3340 Min. 2500
Soundness. Pat     Good Good
- Time of setting ,Vicat test
Amount of water used for normal consistency   % 20.75  
Initial setting time   min 130 Min. 60
Final setting time   hr― min 3-05 Max. 10h
- Compressive strength (N/mm2)
Water used   % 50  
3days     31.8 Min. 12.5
7days     45.9 Min. 22.5
28days     60.7 Min. 42.5

All tests made in accordance with European Standard Specification EN197-1:2000.Strength Class 52.5N.
The above test results comply with EN Specification Requirements for Portland Cement.

Chemical Analysis

Magnesium oxide MgO % 1.04 Max. 5.0
Sulfur trioxide SO3 % 2.06 Max. 3.5
Loss on ignition ig.loss % 1.87 Max. 5.0
Alkalies Na2+0.658K2O % 0,50 Max. 0.75
Chlorine Cl % 0.022 Max. 0.035

All tests made in accordance with European Standard Specification EN197-1:2000.Strength Class 52.5N.
The above test results comply with EN Specification Requirements for Portland Cement.